detail view sample V14_004
treatment method: | Einstufige PEG-Konservierung |
Conservation Laboratory: | Natmus Kopenhagen |
![]() |
wet weight | 1656 g | weight under water | 179 g | ||||
weight after impregnation | no value | weight after drying | 974.5 g | ||||
Umax | 208.0 % | degree of degradation | 2 | ||||
residual density | 0.36 g/cm3 | volume (water displacement) | 1477.0 cm3 | ||||
density before conservation | 1.13 g/cm³ | final density | 0.69 g/cm³ | ||||
impregnation | no value | proportion of impregnating agent | 41.6 % |
nail spacing | before | after | shrinkage |
radial | 66.2 mm | 63.9 mm | 3.4 % |
tangential | 47.8 mm | 45.8 mm | 4.1 % |
longitudinal | 94.1 mm | 93.7 mm | 0.4 % |
volume shrinkage: | 7.7 % |
ASE-radial | 66.5 % | ASE-tangential | 75.6 % |
ASE-longitudinal | 74.5 % | ASE volume | 70.7 % |
volume (previous state) | 1468.1 cm3 | volume (final state) | 1422.4 cm3 | volume shrinkage | 3.1 % |
surface (previous state) | 770.4 cm2 | surface (final state) | 747.4 cm2 | Surface change | -3.0 % |
radial cut surface (previous state) | 9469.3 mm2 | radial cut surface (final state) | 9308.9 mm2 | radial shrinkage | 1.7 % |
tangential cut surface (previous state) | 8395.5 mm2 | tangential cut surface (final state) | 8366.8 mm2 | tangential shrinkage | 0.3 % |
longitudinal measurement (previous state) | 132.0 mm | average length change | -0.0 mm | longitudinal shrinkage | -0.0 % |
ASE-radial | 94.1 % | ASE-tangential | 99.2 % |
ASE-longitudinal | 105.1 % | ASE volume | 93.2 % |
![]() ![]() ![]() ![]() ![]() ![]() ![]() |
pretreatment | Keine weitere Vorbehandlung | |
impregnation | impregnant: | PEG 2000, 10-40%-Lösung mit Leitungswasser |
impregnation process: | Einlegen der Hölzer in 10%-PEG 2000-Lsg., steigern der Konzentration bis auf 40%, keine zusätzliche Erwärmung der Bäder - Tränkung bei Raumtemperatur | |
drying | Gefriertrocknung in gekühlter Kammer (ca. -30°C) | |
aftercare | Entfernen des PEG-Überschusses von der Oberfläche mit weichem Pinsel und Ethanol, nachträgliche Oberflächenfestigung mit 25%iger PEG 2000-Lsg. in Ethanol |
duration pretreatment | no value | duration impregnation | 182 weeks | duration drying | 30 weeks |
total duration of conservation: | 212 weeks |